Abstract
Ensembles of fcc nickel nanowires have been synthesized with defined mean sizes in the interior of single-wall carbon nanotubes. The method allows the intrinsic nature of single-domain magnets to emerge with large coercivity as their size becomes as small as the exchange length of nickel. By means of X-ray magnetic circular dichroism we probe electronic interactions at nickel-carbon interfaces where nickel exhibit no hysteresis and size-dependent spin magnetic moment. A manifestation of the interacting two subsystems on a bulk scale is traced in the nanotubeâs magnetoresistance as explained within the framework of weak localization.
Similar content being viewed by others
Introduction
Magnetic metal clusters continue to attract focus in a broad range of research fields from low dimensional physics1,2,3,4,5,6, chemistry7 to biotechnology8. Magnetic nanostructures have been proven to impact their electronic conduction. The discovery of giant magnetoresistance in layered heterogeneous magnetic systems is a prime example that led to the horizon of new technology based on magnetic nanostructures in semiconductor industry9,10. The magnetism of nanoscale magnetic devices such as spin transfer torques are the forefront of research in spintronics11. While the fundamental properties of freestanding1,3 or supported clusters3,4,5 have been sought, even down to atomistic scales6, it remains a challenge to encapsulate small magnets in advanced electrical materials and control both the bulk magnetism and magnetotransport properties as desired. Of great importance to this end is the understanding of a causal relationship between changes in magnetic properties on a nanoscale and transport properties on a bulk scale.
In this contribution we report a neat method for magnetic nanostructuring within a single-wall carbon nanotube (SWCNT)12,13,14,15,16,17,18, that is an advanced conductor with tunable metallicity19,20. Ensembles of fcc nickel nano clusters have been produced in designer mean dimensions inside SWCNT bundles. The method allows clusters to be formed in situ with dimensions smaller than the exchange length of nickel21. In such a condition the intrinsic nature of single-domain magnets and their advanced magnetism with large coercivity can be exploited as well as the size effects evaluated with no environmental factors.
From transmission electron microscopy (TEM), X-ray diffraction and bulk magnetization measurements we first show that the nickel clusters are controlled in size and exhibit superparamagnetism that manifests itself as spin glass-like states at low temperatures whose net magnetization is reduced at most upon cooling without an external magnetic field (zero field cooling). The hysteretic behaviours, i.e. finite coercivity and superparamagnetic blocking temperature, are scaled by the cluster size. The coercivity become as large as ~42.5âmT for the smallest cluster, much larger than around 0.1âmT of bulk nickel22. The enhanced coercivity strongly supports the formation of single domain magnets.
X-ray magnetic circular dichroism (XMCD) is an exclusive method that allows orbital and spin magnetic moments of minority elements in compounds and alloys to be evaluated23,24. We show that the smallest clustered nickel encapsulated in SWCNTs exhibit a net magnetic moment much reduced as compared to its bulk value at low temperatures. Importantly, no hysteretic effects are observed with XMCD which suggests nickel spins interacting strongly with conduction electrons of SWCNTs, provided that the XMCD probes predominantly surface atoms due to the electron mean free path25. Indeed, the formation of magnetic clusters inside the tubular structure is found to impact the SWCNTâs electronic conduction as well as magnetotransport properties. It is found that the sheet resistance is increased while the low temperature magnetoresistance, known to be negative due to weak localization, is reduced substantially after the cluster formation. Understanding and endohedral control of the bulk magnetism and magnetotransport properties demonstrated in this study would pave the way towards the production of advanced nanomagnets to be applied in spintronics.
Results
Structure
Figure 1 show annular dark field (ADF) scanning transmission electron microscopy (STEM) images for Ni(II) acetylacetonate-filled SWCNT samples annealed in vacuum at 500â°C for 2âhours (a,b) and 700â°C for 2âhours (c,d). In both cases metallic nickel clusters are observed as bright contrasts inside bundled SWCNTs, see electron energy loss spectroscopy (EELS) data in Supplementary Information (SI). Importantly, there exist less, but longer clusters after annealing at 700â°C, representing that the mean cluster size can be controlled with the annealing temperature. The high-resolution micrographs in panel b and d reveal that the elongated clusters are well crystalline, while the short ones can be amorphous.
Bulk magnetism
Figure 2b shows the normalized bulk magnetization isotherms measured at 5âK, for nickel clusters encapsulated in SWCNTs with mean cluster sizes of ~3, 7 and 10ânm evaluated from X-ray diffraction measurements. The numerical value has to be seen as a relative measure for the mean cluster size and not an absolute one, as each sample contains nickel clusters with a finite size distribution as observed in the STEM images. See SI for further discussion. No ferromagnetic impurities have been detected in the pristine SWCNTs. The coercive fields are 42.5, 42.2 and 38.5âmT for the 3, 7 and 10ânm clusters, larger for smaller clusters. Importantly, they are significantly larger as compared to less than 1âmT for bulk nickel, suggesting that nickel clusters are of single domain.
The temperature dependence of the magnetization measured in 100âmT, Fig. 3, exhibits hysteretic behaviour upon zero-field (ZFC) and field cooling (FC), characteristic of superparamagnetic materials in which spins of small magnetic domains are frozen to form a spin glass state with a very small net magnetisation upon cooling in zero field while spins are aligned to exhibit a larger net magnetization upon cooling in a finite field. In the former case, the blocking temperature TB at which the magnetization exhibits a maximum can be defined. We obtain TBâ=â18, 40 and 42âK for the 3, 7 and 10ânm clusters that can be inversely scaled by the cluster length as plotted in the Fig. 3a inset26,27, qualitatively consistent with the previous works on supported ferromagnetic clusters of larger diameters in a range of 2â80ânm28,29,30,31.
The Ni 3d magnetic moments vs temperature measured by XMCD (open rectangles).
The bulk magnetization data measured after zero-field (blue curves) and field cooling (green curves) by SQUID and normalized to the XMCD data at high temperatures. Inset: the blocking temperature versus the reciprocal of the cluster length.
Ni 3d orbital and spin magnetism
Encapsulated in SWCNTs, the single domain nickel clusters arenât affected by environmental factors, allowing these heterogeneous nanostructures to become stable hard magnets. Magnetic properties of each cluster are dominated by the size effect as well as SWCNT-cluster interactions at metal-carbon interfaces. Both together can be accessed exquisitely via XMCD that is intrinsically a surface sensitive method25,32.
Figure 4a shows two X-ray absorption (XAS) spectra μ+ and μâ of the 3ânm cluster collected at the Ni L3,2 edges with photon spins parallel (+) and anti-parallel (â) to the direction of the magnetic field applied to the sample, respectively. Both Ni L3,2 peaks are skewed right and the 6âeV satellite is observed at about 859âeV, characteristic of metallic nickel. The XMCD spectrum is the difference between them, Îμâ=âμ+âââμâ. The orbital ħ and spin
ħ magnetic moments per nickel 3d hole can be derived by using the sum rules33,34,35:

and

where nh is the number of holes in the Ni 3d states, p and q are the area intensities of a μ+âââμâ spectrum over the Ni L3 and L2 edge, respectively and r is the area intensity of a μ+â+âμâ spectrum over the Ni L3,2 edges, see the Fig. 4a inset. The magnetic dipole term ħ in the spin sum rule, where
is the expectation value of the magnetic dipole operator, can be omitted36,37. A degree of circular polarization of 90â±â2% has been taken into account.
Superposed onto the SQUID data in Fig. 3 are the 3d magnetic moments derived from the XMCD data plotted against temperature. The two data sets can be compared since the spin polarization of the Ni 4s and 4p bands is very small35,38. Unlike the SQUID data no difference was observed between the ZFC and FC data. The XMCD probes more atoms on the surface than in the bulk because of the mean free path of low energy electrons25. This applies even if the cluster diameter is as small as 1â2ânm32. In such a case, spin fluctuation as a result of metal spins scattered at the interface by conduction electrons of SWCNTs could influence the degree of the magnetic moment rather than the static spin-glass like disorder which is indeed invisible via XMCD. Note that this fluctuation is more pronounced in the smallest cluster, suggesting the emerging effect of the reduced dimension.
Further in contrast to the SQUID observations (Fig. 2b), the total magnetic moment isotherms estimated from XMCD data vs external magnetic field H (Fig. 4b) show no magnetic hysteresis within the limits of experimental error. This indicates that nickel surfaces are much softer than the bulk as if a hard core-soft shell magnetic structure exist within a cluster.
A quantitative analysis of the magnetization curve as a function of both the applied field and temperature is a difficult task due to the large magnetic anisotropy in crystalline nickel as well as grain size-dependent properties, that cannot be reproduced universally by a theoretical model. Yet, as seen in the Fig. 4b inset in which the magnetization data at 5âK normalized to the maxima are plotted logarithmically against the magnetic field, the initial permeability increases monotonically with increasing the cluster size. The same trend was observed in the previous work on one-order larger diameter ferromagnetic particles at room temperature29, but our data saturate in a much lower field, suggesting a higher degree of magnetic ordering.
The saturation values for the spin and orbital magnetic moments obtained at 5âK and 6âT can be regarded as the spin and orbital magnetic moments in the ground state provided that variations in magnetic moments are very small below 5âK and above 6âT. As summarized in Table 1, we obtain mspinâ~â0.41, 0.48 and 0.50 μB for the 3, 7 and 10ânm clusters, respectively, while morbâ~â0.077, 0.072 and 0.079 μB. The previously reported values for bulk fcc Ni are â=â0.05â0.06,
â=â0.27â0.29, total moment mtotâ=âmorbâ+âmspinâ=â
â=â0.60â0.6239,40, Table 1. Obviously, the spin magnetic moments are reduced from the bulk value. The same trend was observed in thin films40,41, that is in contrast to the case for freestanding nickel clusters in which the magnetic moment increases as the cluster becomes smaller1,42. This is inline with the temperature dependent data, Fig. 3 and is a clear signature of quenched magnetization at low temperatures as a result of interactions in the solid.
As can be noticed from equation 1 and 2, the ratio between the orbital and spin magnetic moments is independent of the hole number nh, hence provides a more precise measure on the Ni 3d ground state when the hole number is not exactly known or could vary. The bulk values reported are morb/mspinâ=ââ~â0.134,40,43. We have morb/mspinâ~â0.19 for the 3ânm cluster which is much larger than ~0.15 and 0.16 for the 7 and 10ânm clusters, respectively. Although the latter values are still larger than ~0.1 for fcc Ni, the much larger value for the smallest cluster is mainly due to the
suppressed by up to 25% while the
values are equally higher than the bulk value within the limits of experimental error.
Similar observations were made in few layer Ni films with values as high as morb/mspinâ~â0.5441 or ~0.36â0.3940, that could be attributed to the reduced coordination number of surface atoms concomitant with regaining spin-orbital coupling. In our system, only spins are enhanced. There is electron transfer from nickel to carbon that leads to the chemical stability of the metallic nickel18. Interactions at the interface could be responsible for the spin suppression, not only those mentioned above.
Magnetotransport
The magnetism as probed by surface sensitive XMCD should predominantly exist at the interface between the clusters and SWCNTs. If so, all changes caused in the interface Ni spins should be observed via the SWCNTâs conduction electrons in contact. Apparently, the interaction is strongest for the smallest cluster in which the spin polarization is largely reduced at low temperatures, see Table 1. This would naturally impact the electronic conduction of SWCNTs, hence in the following we discuss on their magnetotransport properties.
The resistance has been measured as a function of temperature without and with magnetic fields up to ~1âT applied to a direction normal to the current direction. The SWCNTâs electronic conduction can be explained within the variable range hopping (VRH) model as the resistance vs temperature T follows exp(Tâ1/(nâ+â1)) where nâ=â3 corresponds to the dimensionality, the Fig. 5a inset.
(a) Normalized resistance and magnetoresistance (MR) plotted against temperature. In the inset the resistance in logarithmic scale versus Tâ1/4 follows the VRH model (dashed grey lines). (b) Magnetoresistance vs magnetic field at 9.5âK, fitted to Eq. 3 (solid curves).
The magnetoresistance is defined by: M(T, B)â=â[R(T, B)âââR(T, 0)]/R(T, 0), where R(T, B) is the resistance at temperature T and magnetic field B and hence R(T, 0) in zero field. In low fields Bâ<â0.1âT where hysteretic spin glass states emerge at low temperatures, the SWCNT film containing nickel clusters shows only a faint magnetoresistance, which means that the spin disorder among magnetic clusters observed below the blocking temperature in ZFC magnetisation measurements hardly affect the magnetotransport, otherwise alternating direction of cluster spins should give rise to a pronounced negative magnetoresistance if conduction electrons get spin polarized within each magnetic domain. This supports our conclusion that cluster spins interact with conduction electrons only at the metal-carbon interfaces where there is no magnetic order.
Figure 5b shows the field dependence of M(T, B) measured at 9.5âK. The magnetoresistance stays negative and increases as the field increases. No hysteresis observed in the magnetoresistance upon bipolar field scans within ±1âT support the above-mentioned conclusion that the negative magnetoresistance does not originate from the spin dependent electron scattering, nor the domain wall scattering44, since hysteretic features are usually observed near the coercive field.
The field dependence can be fitted well to the following function predicted for a weakly localized three dimensional system45:

where and
, where D is diffusion coefficient and Ïε the energy relaxation time of an electron due to inelastic scattering.
Discussion
The negative magnetoresistance observed for the SWCNT sheet at low temperatures can be understood as a result of weak localization associated with enhanced backscattering when the elastic scattering dominates the electron conduction, as expected and previously observed for carbon nanotube films in similar field ranges. In higher fields a positive magnetoresistance is known to dictate due to the shrinkage of wave functions within the variable range hopping regime46,47.
Upon the encapsulation of nickel clusters the negative magnetoresistance is reduced to 37% of the value for the empty SWCNT as the resistance is increased at low temperatures. The fact that more electron-doped SWCNTs18, containing paramagnetic Ni(II) acetylacetonate (acac) precursor, exhibit the magnetoresistance very similar to the pristine SWCNT, see Fig. 5, leads us to a conclusion that doping of SWCNTs does not take a major role in reducing the magnetoresistance. Indeed, both electron and hole doping of CNTs reportedly lead to a more negative magnetoresistance46. The degree of weak localization can be reduced as a result of an excess phase acquired by a conduction electron via the inclusion of ferromagnetic clusters. This scenario is backed up by the fact that the encapsulation of the paramagnetic Ni(II) acetylacetonate precursor hardly alters the magnetoresistance of SWCNTs.
To conclude, we have demonstrated that the nickel nanomagnets created in SWCNTs outperform their bulky counterparts. With SWCNTsâ advanced properties (high electrical mobility, tuneable energy gap, extremely light weight, flexible and transparent) the method allows nanomagnets to be implemented in various materials and devices. A large change in diffusive conduction of SWCNT webs via the inclusion of nanomagnets indicates much greater impact on the ballistic transport of a single SWCNT that are yet to be studied. A deeper understanding of the magnetic interaction at the metal-carbon interface gained in the present study would help us overcome the superparamagnetic limit in magnetic recording48.
Methods
Sample preparations
The SWCNT films were filtered out of an ethanol solution of an e-Dips SWCNT material with tube diameters of 1.7â±â0.1ânm49, then annealed in high vacuum at 1300â°C for ca. 18âhours so that no magnetic catalysts were detected afterwards by XRD, SQUID and XPS. Nickel clusters were prepared inside SWCNTs via filling with Ni(II) acetylacetonate, molecular formula C10H14NiO4, followed by heating in vacuum: The filling process was commenced by heating the SWCNT film in air at 400â°C for 30âminutes and subsequently in vacuum for 2âhours. Then, the SWCNT film was sealed together with Ni(II) acetylacetonate powder (Sigma Aldrich) in an evacuated glass ampule. The sealed ampule was heated at 130â°C for 8 days12,18, that allows the SWCNT film to be exposed to a vapour of the Ni(II) acetylacetonate. The molecules encapsulated inside SWCNTs can be transformed by heating in vacuum to metal clusters that then act as a catalyst for the formation of inner-shell carbon nanotubes. Hence, whether or not the molecules are encapsulated inside SWCNT can be judged by observing the formation of double-walled carbon nanotubes (DWCNTs). A piece of the film collected from the ampoule was heated in vacuum at temperatures higher than 500â°C and the radial breathing mode (RBM) lines were observed by Raman spectroscopy, see SI. The clusterâs mean length was controlled by varying the heating temperature and determined from XRD measurements. For XMCD and SQUID measurements three different samples were cut out from one Ni(II) acetylacetonate-filled SWCNT sheet and annealed in vacuum at 500â°C for 2âhours, 700â°C for 2âhours, or 800â°C for 5âhours. For magnetotransport measurements stripes (~2âmmâÃâ10âmm) of SWCNTs with and without filling of nickel, before and after annealing in vacuum at 500° C for 2âhours were prepared. Four point probe contacts were made by pressing gold wires onto the SWCNT stripe.
Experimental methods
Nickel-filled SWCNT samples were dispersed in n-hexane by sonication and dropped onto molybdenum microgrids covered with holey amorphous carbon films for STEM. ADF-STEM images were obtained by using a JEOL JEM-2100F microscope equipped with Delta spherical aberration correctors at an electron accelerating voltage of 60âkV50. Electron energy loss spectroscopy was performed by using a Gatan Quantum spectrometer installed into the microscope.
XRD measurements were carried out at a Bruker Nanostar equipped with a pinhole camera, a 2D gas detector (Vantec 2000) and an image plate (Fuji FLA 7000) for simultaneous measurement of small-angle and wide-angle X-ray scattering patterns. The X-ray patterns were radially averaged to obtain the scattering intensities in dependence on the scattering vectorâ=â4Ïsin(θ)/λ, where 2θ is the scattering angle and λâ=â0.1542 nm the X-ray wavelength.
The Raman data were recorded at room temperature using a Bruker FT Raman spectrometer with an excitation energy (wavelength) of 1.16âeV (1064ânm). Bulk magnetisation measurements were carried out at Atominstitut, Vienna University of Technology, using a SQUID magnetometer with magnetic fields up to 1âT and temperatures in a range of 5 to 300âK. XMCD measurements were carried out at UE46-PGM-1 variable polarization undulator beamline at BESSY II synchrotron facility, Helmholtz-Zentrum Berlin (HZB). XMCD spectra were recorded by measuring the sample drain current over the Ni 2p edge with the photon helicity parallel (μ+) or antiparallel (μâ) to the magnetic field applied to the sample. The experimental end-station of this beamline allowed cooling the sample down to 5âK in magnetic fields up to 6âT.
The resistance was measured in four point geometry at temperatures ranging from 9 to 310âK and in external magnetic fields up to 1âT in a setup equipped with a closed-cycle helium cryocooler with the sample attached onto a temperature-controlled cold finger in vacuum. The data were collected with the magnetic field applied normal to the current direction. Switching the magnetic field orientation parallel to the current direction caused no change in the resistance and magnetoresistance. This confirms that the Lorentz force on the carrier doesnât lead to a significant contribution to the magnetoresistance.
Additional Information
How to cite this article: Shiozawa, H. et al. Nickel clusters embedded in carbon nanotubes as high performance magnets. Sci. Rep. 5, 15033; doi: 10.1038/srep15033 (2015).
References
Billas, I. M. L., Chatelain, A. & Deheer, W. A. Magnetism from the atom to the bulk in iron, cobalt and nickel clusters. Science 265, 1682â1684 (1994).
Shi, J., Gider, S., Babcock, K. & Awschalom, D. D. Magnetic clusters in molecular beams, metals and semiconductors. Science 271, 937â941 (1996).
Tiago, M. L., Zhou, Y., Alemany, M. M. G., Saad, Y. & Chelikowsky, J. R. Evolution of magnetism in iron from the atom to the bulk. Physical Review Letters 97, 147201 (2006).
Gambardella, P. et al. Ferromagnetism in one-dimensional monatomic metal chains. Nature 416, 301â304 (2002).
Gambardella, P. et al. Giant magnetic anisotropy of single cobalt atoms and nanoparticles. Science 300, 1130â1133 (2003).
Khajetoorians, A. A. & Wiebe, J. Hitting the limit of magnetic anisotropy. Science 344, 976â977 (2014).
Santra, S. et al. Synthesis and characterization of silica-coated iron oxide nanoparticles in microemulsion: The effect of nonionic surfactants. Langmuir 17, 2900â2906 (2001).
Alivisatos, P. The use of nanocrystals in biological detection. Nature Biotechnology 22, 47â52 (2004).
Baibich, M. N. et al. Giant magnetoresistance of (001)fe/(001) cr magnetic superlattices. Physical Review Letters 61, 2472â2475 (1988).
Binasch, G., Grunberg, P., Saurenbach, F. & Zinn, W. Enhanced magnetoresistance in layered magnetic-structures with antiferromagnetic interlayer exchange. Physical Review B 39, 4828â4830 (1989).
Ralph, D. C. & Stiles, M. D. Spin transfer torques. Journal of Magnetism and Magnetic Materials 320, 1190â1216 (2008).
Shiozawa, H. et al. A catalytic reaction inside a single-walled carbon nanotube. Adv. Mater. 20, 1443â1449 (2008).
Shiozawa, H. et al. Fine tuning the charge transfer in carbon nanotubes via the interconversion of encapsulated molecules. Phys. Rev. B 77, 153402 (2008).
Shiozawa, H. et al. Screening the missing electron: Nanochemistry in action. Phys. Rev. Lett. 102, 046804 (2009).
Shiozawa, H. et al. Filling factor and electronic structure of dy3n@c-80 filled single-wall carbon nanotubes studied by photoemission spectroscopy. Phys. Rev. B 73, 205411 (2006).
Shiozawa, H. et al. Catalyst and chirality dependent growth of carbon nanotubes determined through nano-test tube chemistry. Advanced Materials 22, 3685â3689 (2010).
Briones-Leon, A. et al. Orbital and spin magnetic moments of transforming one-dimensional iron inside metallic and semiconducting carbon nanotubes. Physical Review B 87, 195435 (2013).
Kharlamova, M. V. et al. Doping of single-walled carbon nanotubes controlled via chemical transformation of encapsulated nickelocene. Nanoscale 7, 1383â1391 (2015).
Arnold, M. S., Green, A. A., Hulvat, J. F., Stupp, S. I. & Hersam, M. C. Sorting carbon nanotubes by electronic structure using density differentiation. Nature Nanotechnology 1, 60â65 (2006).
Liu, H., Nishide, D., Tanaka, T. & Kataura, H. Large-scale single-chirality separation of single-wall carbon nanotubes by simple gel chromatography. Nature Communications 2, 309 (2011).
Ashcroft, N. W. & Mermin, N. D. Solid State Physics (Saunders College Publishing, 1976).
Nakamura, Y. Residual magnetization and magnetostriction of nickel single crystals. Journal of the Physical Society of Japan 10, 937â971 (1955).
Schutz, G. et al. Absorption of circularly polarized x-rays in iron. Physical Review Letters 58, 737â740 (1987).
Shiozawa, H. et al. Local magnetic susceptibility in rare-earth compounds. Journal of the Physical Society of Japan 72, 2079â2084 (2003).
Seah, M. P. & Dench, W. A. Quantitative electron spectroscopy of surfaces: a standard data base for electron inelastic mean free paths in solids. Surface and Interface Analysis 1, 2â11 (1979).
Herzer, G. Grain-size dependence of coercivity and permeability in nanocrystalline ferromagnets. Ieee Transactions On Magnetics 26, 1397â1402 (1990).
Loffler, J. F., Meier, J. P., Doudin, B., Ansermet, J. P. & Wagner, W. Random and exchange anisotropy in consolidated nanostructured fe and ni: Role of grain size and trace oxides on the magnetic properties. Physical Review B 57, 2915â2924 (1998).
Morup, S. & Tronc, E. Superparamagnetic relaxation of weakly interacting particles. Physical Review Letters 72, 3278â3281 (1994).
Perez, J. A. L., Quintela, M. A. L., Mira, J., Rivas, J. & Charles, S. W. Advances in the preparation of magnetic nanoparticles by the microemulsion method. Journal of Physical Chemistry B 101, 8045â8047 (1997).
Chen, Q. & Zhang, Z. J. Size-dependent superparamagnetic properties of mgfe2o4 spinel ferrite nanocrystallites. Applied Physics Letters 73, 3156â3158 (1998).
Liu, C. & Zhang, Z. J. Size-dependent superparamagnetic properties of mn spinel ferrite nanoparticles synthesized from reverse micelles. Chemistry of Materials 13, 2092â2096 (2001).
Shiozawa, H. et al. Photoemission and inverse photoemission study of the electronic structure of c-60 fullerenes encapsulated in single-walled carbon nanotubes. Physical Review B 73, 075406 (2006).
Thole, B. T., Carra, P., Sette, F. & van der Laan, G. X-ray circular-dichroism as a probe of orbital magnetization. Physical Review Letters 68, 1943â1946 (1992).
Carra, P., Thole, B. T., Altarelli, M. & Wang, X. Physical Review Letters 70, 694â697 (1993).
Chen, C. T. et al. Experimental confirmation of the x-ray magnetic circular-dichroism sum-rules for iron and cobalt. Physical Review Letters 75, 152â155 (1995).
Komelj, M., Ederer, C., Davenport, J. W. & Fahnle, M. From the bulk to monatomic wires: An ab initio study of magnetism in co systems with various dimensionality. Physical Review B 66, 140407 (2002).
Peredkov, S. et al. Spin and orbital magnetic moments of free nanoparticles. Physical Review Letters 107, 233401 (2011).
Eriksson, O., Fernando, G. W., Albers, R. C. & Boring, A. M. Enhanced orbital contribution to surface magnetism in fe, co and ni. Solid State Communications 78, 801â806 (1991).
Eriksson, O., Johansson, B., Albers, R. C., Boring, A. M. & Brooks, M. S. S. Orbital magnetism in fe, co and ni. Physical Review B 42, 2707â2710 (1990).
Vogel, J., Panaccione, G. & Sacchi, M. X-ray-absorption study of the magnetic-moments in thin ni layers on fe(100). Physical Review B 50, 7157â7160 (1994).
Dhesi, S. S., Durr, H. A., van der Laan, G., Dudzik, E. & Brookes, N. B. Electronic and magnetic structure of thin ni films on co/cu(001). Physical Review B 60, 12852â12860 (1999).
Apsel, S. E., Emmert, J. W., Deng, J. & Bloomfield, L. A. Surface-enhanced magnetism in nickel clusters. Physical Review Letters 76, 1441â1444 (1996).
Chen, C. T., Sette, F., MA, Y. & Modesti, S. Soft-x-ray magnetic circular-dichroism at the l2,3 edges of nickel. Physical Review B 42, 7262â7265 (1990).
Gregg, J. F. et al. Giant magnetoresistive effects in a single element magnetic thin film. Physical Review Letters 77, 1580â1583 (1996).
Kawabata, A. Theory of negative magnetoresistance in 3-dimensional systems. Solid State Communications 34, 431â432 (1980).
Takano, T., Takenobu, T. & Iwasa, Y. Enhancement of carrier hopping by doping in single walled carbon nanotube films. Journal of the Physical Society of Japan 77, 124709 (2008).
Yanagi, K. et al. Transport mechanisms in metallic and semiconducting single-wall carbon nanotube networks. Acs Nano 4, 4027â4032 (2010).
Skumryev, V. et al. Beating the superparamagnetic limit with exchange bias. Nature 423, 850â853 (2003).
Saito, T. et al. Selective diameter control of single-walled carbon nanotubes in the gas-phase synthesis. Journal of Nanoscience and Nanotechnology 8, 6153â6157 (2008).
Sasaki, T. et al. Performance of low-voltage stem/tem with delta corrector and cold field emission gun. Journal of Electron Microscopy 59, S7âS13 (2010).
Acknowledgements
We acknowledge the Helmholtz-Zentrum Berlin - Electron storage ring BESSY II for provision of synchrotron radiation at beamline UE46/PGM-1 and would like to thank Dr. Enrico Schierle for assistance. This work was supported by the Austrian Science Funds (FWF), projects P621333-N20 and P27769-N20. Y.S. and K.S. acknowledge financial support from JSPS KAKENHI (grant number 25410246) and JST Research Acceleration Program. We thank S. Loyer and A. Stangl for technical assistance.
Author information
Authors and Affiliations
Contributions
H.S. conceived and designed the experiments. H.S., A.B.L., O.D. and T.S. prepared the samples. H.S., A.B.L., G.Z., O.D., Y.S., K.S., M.E., E.W. and H.P. performed the experiments. H.S., A.B.L., O.D. and H.P. analysed the data. H.S., W.L., H.P. and T.P. wrote and reviewed the manuscript.
Ethics declarations
Competing interests
The authors declare no competing financial interests.
Electronic supplementary material
Rights and permissions
This work is licensed under a Creative Commons Attribution 4.0 International License. The images or other third party material in this article are included in the articleâs Creative Commons license, unless indicated otherwise in the credit line; if the material is not included under the Creative Commons license, users will need to obtain permission from the license holder to reproduce the material. To view a copy of this license, visit http://creativecommons.org/licenses/by/4.0/
About this article
Cite this article
Shiozawa, H., Briones-Leon, A., Domanov, O. et al. Nickel clusters embedded in carbon nanotubes as high performance magnets. Sci Rep 5, 15033 (2015). https://doi.org/10.1038/srep15033
Received:
Accepted:
Published:
DOI: https://doi.org/10.1038/srep15033